Qinhuangdao Haichi Technology & Trade Co., Ltd
|
|
| |
|
|
|
|

|
|
|
High Temperature and corrosion resistent Inconel
Composition of Inconel(Wt%竊�span lang="EN-US">
|
Material Grade
|
Ni
|
Cr
|
Fe
|
Si
|
Mn
|
Co
|
Cu
|
Al
|
Ti
|
Mo
|
other
|
|
Inconel 600
|
≥72
|
14/17
|
6/10
|
≤0.5
|
≤1.0
|
|
≤0.5
|
|
|
|
C≤0.15
|
|
Inconel 601
|
58/63
|
21/25
|
balance
|
≤0.5
|
≤1.0
|
|
≤1.0
|
1.0-1.7
|
|
|
C≤0.1
|
|
Inconel 625
|
≥58
|
20/23
|
5.0
|
≤0.5
|
≤0.5
|
≤1.0
|
|
≤0.4
|
≤0.4
|
8-10
|
Nb3.15/4.15
|
|
Inconel 686
|
balance
|
19/23
|
1.0
|
≤0.08
|
≤0.75
|
|
|
|
≤0.25
|
15-17
|
W3.0/4.4
|
|
Inconel 690
|
≥58
|
27/31
|
7/11
|
≤0.5
|
≤0.5
|
|
≤0.5
|
|
|
|
|
|
Inconel 718
|
50/55
|
17/21
|
balance
|
≤0.35
|
≤0.35
|
≤1.0
|
≤0.3
|
≤0.9
|
≤1.15
|
2.8/3.3
|
Nb4.75/5.5
|
|
Inconel 751
|
≥70
|
14/17
|
5/9
|
≤0.5
|
≤0.1
|
|
≤0.5
|
≤1.5
|
≤2.6
|
|
Nb1.2
|
|
Inconel 783
|
26/30
|
2.5/3.5
|
24/27
|
≤0.5
|
≤0.5
|
balance
|
|
≤5.6
|
≤0.3
|
|
Nb3.5
|
|
Inconel 800
|
30/35
|
19/23
|
≤39.5
|
≤1.0
|
≤1.5
|
|
≤0.75
|
≤0.6
|
≤0.6
|
|
|
|
Inconel 803
|
32/37
|
25/29
|
balance
|
≤1.0
|
≤1.5
|
|
≤0.75
|
≤0.6
|
≤0.6
|
|
|
|
Inconel 825
|
38/46
|
19.5/23.5
|
≤22
|
≤0.5
|
≤1.0
|
|
≤3.0
|
≤0.2
|
≤1.2
|
≤3.5
|
|
|
Inconel 864
|
30/38
|
20/25
|
balance
|
≤1.0
|
≤1.0
|
|
|
≤1.0
|
≤1.0
|
≤4.8
|
|
|
Inconel 903
|
36/40
|
|
balance
|
|
|
13/17
|
|
≤1.15
|
≤1.85
|
|
Nb≤3.5
|
|
Inconel 908
|
47/51
|
3.75/4.5
|
balance
|
≤0.50
|
≤1.0
|
|
≤0.5
|
≤1.25
|
≤1.80
|
≤0.5
|
Nb≤3.3
|
|
Inconel 909
|
35/40
|
|
|
≤0.50
|
|
12/16
|
|
≤0.15
|
≤1.80
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Mechanical Properties of Inconel
|
Material Grade
|
Tensile strength
|
Yield Strength
|
Elongation
|
Tempering
|
|
閨b竊�/span>Mpa竊�/span>
|
閨0.2竊�/span>Mpa竊�/span>
|
δ5(%)
|
|
Inconel600
|
655
|
310
|
40
|
Soft annealed
|
|
Inconel625
|
812
|
345
|
42
|
Soft Annealed
|
|
Inconel718
|
1320
|
1100
|
20
|
�뜻���/span>
|
|
Inconel800
|
552
|
290
|
40
|
Soft Annealed
|
|
Inconel825
|
696
|
286
|
40
|
Soft Annealed
|
|
|
|
|
| |
|
|
|